Ceramic Foam Insulation: Where It Fits and Where It Does Not
Ceramic foam insulation earns its place when one rigid board must deliver A1 non-combustibility, compressive strength and negligible water absorption at the same point in a build-up — slab-edge barriers, plinths, soffits, machined thermal breaks. It is the wrong answer where wall depth is fixed and the U-value target is demanding: a sintered ceramic foam board conducts about 1.9 times as much heat per millimetre as a mineral wool slab at the midpoint of each published range. Two figures decide it: declared conductivity and available thickness.
Two materially different products are sold under one name.
The first is a sintered closed-pore board. A granted patent describes a body of ceramic tile polishing slag with feldspar, calcined talc, red clay and silicon carbide as foaming agent, fired at 1,130–1,180 °C and cut to size. Because the pores are sealed, it reaches 0.15–0.17 g/cm³ with water absorption at or below 0.5 percent, measured under GB/T 5486-2008.
The second is a cast foam ceramic — clay or loam with fly ash, foamed and fired at 950–1,100 °C — and it is open-porous. A 2025 study in Ceramics reports an optimised mix at 680–700 kg/m³, compressive strength 3.5–4 MPa and conductivity 0.135–0.140 W/(m·K), noting the family spans roughly 0.05–0.15 W/(m·K). It also shows porosity falling from 85 to 65 percent between 900 and 1,100 °C.
So the label alone tells a specifier little: density, conductivity and water absorption belong in the clause.
The table sets out what a sintered closed-pore board is documented to achieve, for the sealed-cell family only.
| Property | Documented value | Basis |
|---|---|---|
| Density | 150–170 kg/m³ | Granted patent CN102887721B, tested to GB/T 5486-2008 |
| Thermal conductivity | 0.066–0.078 W/(m·K) | Same patent, same series |
| Compressive strength, ultimate | ≥ 1.5 MPa | Same |
| Water absorption | ≤ 0.5 percent | Same |
| Reaction to fire | Class A1 | Same; criteria per EN 13501-1 |
| Water vapour permeance | 2.01×10⁻⁷ to 2.41×10⁻⁷ g/(m²·s·Pa) | Same; GB/T 17146 |
| Firing temperature, process | 1,130–1,180 °C | Same |
| Maximum service temperature | [TO VERIFY] — read from the product DoP | — |
Two readings matter. The board is roughly twice as dense as a typical mineral wool slab and several times stronger in compression, which is why it can be machined into a load-bearing thermal break. Its 0.066–0.078 W/(m·K) compares with 0.035–0.040 W/(m·K) for mineral wool in a peer-reviewed review — both legitimate, for different jobs.
Under EN 13501-1, class A1 requires EN ISO 1182 to give a temperature rise of no more than 30 °C, mass loss of no more than 50 percent and no sustained flaming, plus a gross calorific potential (EN ISO 1716) of no more than 2.0 MJ/kg. A board meeting those thresholds adds no fuel to a fire. The non-combustibility test is a small-specimen furnace exposure judged on those three criteria alone, and it says nothing about how an assembly behaves.
That is the whole of the claim. A1 states nothing about conductivity, strength, absorption, adhesion or dimensional behaviour. In facade work the consequential questions are about the assembly: curtain wall spandrel configurations are assessed under EN 1364-4, which tests a three-dimensional specimen so the upstand or downstand is exposed as built. That test, plus national height limits and cavity-barrier rules, decides use. A tender saying "A1 insulation" has specified a fire class and left the engineering open.
Four locations justify the premium, and the reason in each is mechanical or hygric.
Slab-edge and spandrel fire barriers in curtain walls. The barrier must be continuous, dimensionally stable and rigid enough to survive installation behind a closed facade. A closed-pore board at 150–170 kg/m³ with compressive strength above 1.5 MPa cuts to the spandrel depth and does not slump.
Plinths and base-of-wall zones. Here an envelope takes driven rain, splash-back and de-icing salt. Absorption at or below 0.5 percent removes the mechanism that usually degrades performance first.
Soffits and undersides. Downward-facing surfaces collect water and are awkward to membrane; a board that stays dry without a separate vapour control layer simplifies the detail.
Machined thermal breaks in framed facades. Where a break is cut to profile and carries bracket load, closed cells, 1.5 MPa strength and machinability are the reason for the choice.
Each case still needs three numbers: compressive strength at the design load, maximum water absorption, fire class.
The limits concern depth and movement, not quality.
Thin walls with demanding U-values. U = 0.20 W/(m²·K) needs 5.0 m²·K/W in total. Allowing 0.30 for surface films and substrate, the insulation must supply about 4.7 m²·K/W: roughly 330 mm at λ = 0.070 W/(m·K), roughly 175 mm at λ = 0.0375 W/(m·K). With 200 mm of depth, the ceramic foam option does not close. Indicative figures — a real calculation uses declared λ — but the order of magnitude decides the detail.
Adhesively fixed systems on flexible substrates. Tensile strength perpendicular to faces (EN 1607) and compression (EN 826) must be designed, not assumed: a rigid board does not follow substrate deflection as a fibrous slab does. On a lightweight framed wall with movement, that effort often outweighs the gains.
Complex and curved geometry. Rigid boards do not drape: every change of plane becomes a cut and a joint, and each joint is a thermal bridge to detail and seal.
Volume-driven budgets. Firing above 1,100 °C is energy-intensive; take embodied carbon from an EPD. Where the only requirement is a U-value across a thick cavity, the fibrous option wins.
Eight checks separate a defensible ceramic foam clause from a vague one, and they take an afternoon with the supplier's documents on file.
- Density given as a range with a tolerance, not a single figure.
- Conductivity declared at a named mean temperature and thickness, taken from the declaration of performance.
- Compressive strength compared with the design load at the detail, not with a generic minimum.
- Water absorption stated as a test method and a limit, not as an adjective.
- Fire class quoted with the standard and the test report reference.
- Tensile strength perpendicular to faces (EN 1607) confirmed where the board is adhesively fixed.
- Joint, fixing and cavity-barrier details drawn rather than described.
- Embodied carbon taken from an EPD and compared on the same functional unit.
If any of the first six cannot be answered from documents, the clause is not yet writable.
Is ceramic foam the same as cellular glass? No. Cellular glass is foamed glass; ceramic foam is a sintered ceramic or glass-ceramic body from clay or ceramic waste. Both are closed-cell and can reach A1, but density, strength and conductivity differ, so data cannot be carried across.
Does A1 mean the board can be used at any building height? No. A1 covers reaction to fire only. Height limits, cavity-barrier rules and system evidence come from national codes and assembly tests such as EN 1364-4.
What thickness do I need for a given U-value? Divide the required thermal resistance by the declared conductivity. At λ = 0.070 W/(m·K), U = 0.20 W/(m²·K) needs about 330 mm once surfaces and substrate are allowed for; at λ = 0.0375 W/(m·K), about 175 mm.
Can it be used where it will be permanently wet? Low absorption is not a drainage design: the board will not take up water as an open-porous material does, but joints, fixings and the assembly must still shed water.
Related product ranges: ceramic foam · rock wool · foam glass · calcium silicate
Working on a facade detail where fire class, depth and load compete? Send the build-up, the U-value target and the barrier location and we will check the thickness and fixing logic against the board data.